A dent and a scratch are different injuries. A dent is compressed fibre, which can often be lifted back out. A scratch is removed fibre, which cannot be put back and has to be sanded level instead. Treating one like the other is why repairs go wrong.

Dents: steam them out

If something heavy was dropped and the wood is crushed rather than cut, the fibres are compressed and still intact. Water and heat make them swell back towards their original shape.

  1. Remove the finish over the dent. Lightly, with a fine abrasive pad, enough that water can reach the wood. Steam cannot get through a cured finish.
  2. Wet the dent with a few drops of water and let it soak in for a minute.
  3. Damp cloth, warm iron. Cotton cloth folded over the dent, iron on a medium setting, a few seconds at a time. You will hear it steam. Lift and check constantly.
  4. Repeat. Several short cycles beat one long one, which scorches.
  5. Let it dry fully, then sand the raised area flat along the grain, working out from the repair so there is no step.
  6. Re-oil the area, then the whole top so the sheen matches.

This works well on oak and plane. Walnut is softer and dents more readily, and also recovers well. It does not work where the fibres were actually cut.

Why this only works on an oiled top

Every step here assumes you can remove the finish locally and blend new finish back in. A hardwax oil lets you do that invisibly. A cured film finish does not: a patch of new lacquer in an old lacquer surface always reads as a patch. On a lacquered top, a dent repair means sanding and refinishing the whole surface.

Scratches: how deep

Run a fingernail across it. If the nail does not catch, the scratch is in the finish only. If it catches, it is in the wood.

DepthFixTime
In the finish, nail does not catchFine abrasive pad along the grain, spot oil, refresh the top20 minutes plus cure
Shallow in the woodSand the area through the grits, feather it out, oilAn hour plus cure
Deep gougeSteam what you can, sand the rest, accept a slight hollowHalf a day
Through to a void or crackTreat as a repair, not a scratchSee crack repair

The rule that makes repairs invisible

Feather the repair out over a wide area. Sanding a 2 cm scratch inside a 3 cm circle leaves a visible dish. Work the same area out to 20 or 30 cm so the transition is gradual and your eye cannot find an edge. Then re-oil the whole top, not just the patch, because fresh oil over old oil is slightly different in sheen until it has all aged together.

Grit matters

Finish the repair at the same grit the top was sanded to, usually 150 to 180. Sanding the patch finer than the surroundings makes it take oil differently and shows as a lighter area, which is the most common way a repair announces itself. See the sanding sequence for a slab top.

What to do first on a new table

Keep an offcut from the same slab, finished the same way, stored somewhere it gets similar light. In three years it is your test piece and your colour reference, and it is the difference between a confident repair and an experiment on the table.

When not to repair

A slab table collects marks and that is part of what it is. A small dent from a dropped pan at a family meal is not damage requiring an afternoon with a sander. Fix the things that catch, snag, hold dirt or expose bare wood. Leave the rest to become the table's history.

Common questions

How do you get a dent out of a wood table?

Sand the finish off the dent lightly, wet it, then apply a warm iron through a damp cloth in short bursts. The compressed fibres swell back. Sand flat when dry and re-oil the area and the top.

Can you repair a scratch on an oiled table?

Yes, and invisibly. Sand the area along the grain, feather it out over 20 to 30 cm, finish at the same grit as the rest of the top, then re-oil the whole surface.

Why does my repair show as a lighter patch?

Usually because the patch was sanded finer than the rest of the top, so it takes less oil. Re-sand the area to the same grit as the original surface and re-oil.

Can a dent be steamed out of a lacquered table?

Not without refinishing. Steam cannot pass through a cured film, and a new patch of film cannot be blended into an old one. The repair is to sand the whole top back.